Step-By-Step Instructions for Mixing Plaster

These instructions are for pottery plaster: Arcosa Pottery Plaster, or USG No. 1 if you still have some. Hydrocal and Hydro-Stone take much less water; see Mixing Hydrocal and Hydro-Stone at the bottom of this page.

Switching from USG No. 1? Mix Arcosa at the same ratio. Read how the two compare.

Note: Always wear a respirator when you work with dry materials!

1. First, figure out your quantities:

Pottery Plaster-to-Water Mixing Chart (100:70 ratio) – Arcosa Pottery Plaster and USG No. 1

Note: Water measurements are approximate. Always mix by weight for precision in professional or mold-making applications. This chart is for pottery plaster only; don't use it for Hydrocal or Hydro-Stone.

Sps plaster to water mixing chart for pottery molds

2. Measure Water:

  • Weigh the water into a clean mixing bucket first. Room-temperature water (70–80 °F) gives the most predictable set; warmer water sets faster.

3. Sift in Plaster:

  • Slowly and evenly sift the plaster into the water so it absorbs without clumping. Don't dump it in all at once.
  • Let it soak without stirring for 2–4 minutes (this is called "slaking"). Small batches need less time than big ones.

4. Mix Thoroughly:

  • Hand mix or use a drill mixer for 2–5 minutes, until smooth and creamy.
  • Keep the mixer blade under the surface so you don't whip in air bubbles.
  • Longer mixing makes a stronger mold but shortens your working time.

5. Pour Immediately:

  • Pour into your mold box or form promptly, in a steady stream, into one corner so it flows across the model.
  • Tap or jiggle the form to bring bubbles to the surface.

6. Allow to Set:

  • Don't disturb it while it sets. Pottery plaster sets in roughly 25–40 minutes and gets warm as it does; once it cools you can demold.
  • Let molds dry completely before you cast in them: usually several days, until the mold no longer feels cool or loses weight. If you use heat, keep it under 120 °F.

7. Clean Up:

  • Never pour plaster or plaster rinse water down a drain. It sets in the pipe.
  • Let leftover plaster harden in the bucket, then flex the bucket to pop it out and throw it in the trash. Rinse tools in a bucket of water and let the sediment settle before you dump the clear water outside.

8. Store Plaster:

  • Close the bag tightly and keep it somewhere dry and off the floor. Plaster absorbs moisture from the air; old or damp plaster sets fast, sets lumpy and makes weak molds.

Mixing Hydrocal and Hydro-Stone

These are gypsum cements: much harder and less absorbent than pottery plaster, for sculpture, master patterns and durable casts. They are not for slip-casting molds. Mix them the same way, by weight, with much less water:

  • Hydrocal (White): 40–45 parts water to 100 parts plaster
  • Hydro-Stone: 32 parts water to 100 parts plaster. A drill mixer gives the strongest casts.

Example: 10 lb of Hydro-Stone takes 3.2 lb of water; 10 lb of pottery plaster takes 7 lb.